W/Si復合材料的制備及抗激光沖擊性能W/Si復合材料的制備及抗激光沖擊性能Preparation and laser shock resistance of W/Si composites 采用機械合金化和放電等離子體燒結(1700 ℃,44.1 MPa)的方法成功制備W/Si復合材料,并通過SEM、EDS、XRD等分析手段以及顯微硬度測試和激光熱沖擊試驗對其組織結構、顯微硬度及抗熱沖擊性能進行研究。結果表明:燒結后試樣隨Si含量的增加依次生成W5Si3和Si2W中間相,該結果與W-Si二元相圖完全吻合。激光沖擊后試樣表面呈現出3種不同形貌:熔融區、影響區及未影響區(邊緣區)。相較于其他試樣,W/5%Si(質量分數)復合材料的晶粒小、硬度高,具有較好的抗熱沖擊性能。 W/Si composites were produced through powder metallurgy and subsequent spark plasma sintering (SPS) at 1700 ℃ and 44.1 MPa. SEM, EDS, XRD analysis, microhardness and laser thermal shock tests were used to characterize these microstructure and properties of W/Si composites. The results show that W5Si3 and Si2W phases generate in sequence with the increase of Si element, which corresponds well with the binary phase diagram of W-Si. The laser irradiated surfaces are roughly divided into three parts: the melting region (the center), unaffected region (the edges), and the affected area (between the two regions). Comparing with different samples, W/5%Si (mass fraction) samples seem to possess the relatively better thermal shock resistance due to the smaller grain size and higher microhardness. 全文下載:https://pan.baidu.com/s/1dGV74Md? 作為值得信賴的合作伙伴和高品質金屬合金的半成品供應商,通項公司擁有完善的服務體系和專業的團隊。在同客戶交易的過程中,我們力求根據不同的應用需求將我們的產品做到精益求精。針對當前和未來的市場需求,通項公司致力于為客戶提供最佳的金屬材料解決方案。 TXCO has been a reliable partner and supplier of sophisticated and high-quality semi-finished products maed of alloys. In dialogue with our customers, we optimise our products to meet the specific application requirements. TXCO develops the best alloy material solutions for current and future challenges. 獲取更多我們供應的產品和服務信息,請致電086-021-6786 0205或發電子郵件service@sinoav.com聯系我們,您也可以通過微信,微博,領英,臉書,推特和谷歌+與我們互動。 For more information on the products and services that we supply, call us at 086-021-6786 0205 or email us at service@sinoav.com. You can also get in touch on social media, we are constantly active on Weixin, Weibo, LinkedIn, Facebook, Twitter and Google+.
|